Close
010-57374441
Support & Services

Common Problems for XRF fusion bead Method

Time : 2022-07-28 Visits : 689

1)XRF fusion bead Preservation

Most XRF fusion bead are somewhat hygroscopic. The most hygroscopic is prepared by Na2B4O7, covered with a layer of white hydrate. Lithium borate flux is less affected by humidity. In any case, samples to be tested should be kept in the dryer, especially the standard material.

2) XRF fusion bead rupture

XRF fusion bead rupture is related to many factors:

3) XRF fusion bead burst

XRF fusion bead with internal stress sometimes burst usually after operation or prolonged cooling. The stability of the glass bead can be increased by adding a small amount of SiO2 or Li2B4O7 to the flux mixture. The factors that cause internal stress are:

4) Crystallization during cooling

XRF fusion bead crystallization is unfavorable, so it should be avoided in preparation. The factors include:

5) Ejecting of melting mixture from the crucible

This problem is caused by humidity, hydration or carbonate and can be solved as follows:

6) The apparent insoluble black spots floating on the bead surface

The black spots indicate the presence of graphite, and handle this as follows:

7)Bubbles continuously formed at the bottom of the crucible

This may be caused by the decomposition of SO3 in the melting body into SO2 gas. The following measures could be taken:

8) Bubbles on the bead surface

If bubbles appear, do as follows:


PREV : Maintenance of water ChillersNEXT : Notes for Crucible Usage